Table 7.2. Directions For Preparing Simulated Muscle Material
For 200-2450 MHz (Guy, 1971a; Chou et al., 1984)
- Weigh all ingredients and determine percentages by weight.
- Mix ingredients except TX-150 in 14-20°C water with a 4-in. shear stirrer rotating at 450 rpm on a variable-speed drill press until all polyethylene powder is wet. Add one drop of household liquid detergent to help wet the polyethylene powder.
- Add TX-150 and increase drill press speed to 1200 rpm.
- Mix for about 45-120 s. When the mixture becomes thick, slow the drill press to about 800 rpm to avoid generating air bubbles. Since the setting time of TX-150 varies with factory batch, proper water temperature and mixing time must be determined by experience. If stirred too long, the mixture will become too hard to pour; if not stirred enough, the polyethylene powder will float.
- Pour the mixture into the mold, slowly, to allow air bubbles to escape from the mixture.
This is a Department of Defense computer system for authorized use only.
DoD computer systems may be monitored for all lawful purposes, including
to ensure that their use is authorized, for management of the system, to
facilitate against unauthorized access, and to verify security procedures,
survivability, and operational security. Using this system constitutes
consent to monitoring. All information, including personal information,
placed on or sent over this system may be obtained during monitoring.
Unauthorized use could result in criminal prosecution.
POC: AFRL/HEDM, (210)536-6816, DSN 240-6816